Chemistry
Data : (化學成分)??
Carbon??0.38 - 0.46??
Chromium??0.7 -
0.95??
Iron??Balance??
Manganese??0.6 - 0.9??
Molybdenum??0.3 -
0.65??
Nickel??1.65 - 2??
Phosphorus??0.01 max??
Silicon??1.45 -
1.8??
Sulphur??0.01 max??
Vanadium??0.05 min??
物理特性
Physical Data
:???
Density (lb / cu.
in.)??0.283??
Specific Gravity??7.83??
Specific Heat (Btu/lb/Deg F -
[32-212 Deg F])??0.116??
Melting Point (Deg F)??2590??
Thermal
Conductivity??21??
Mean Coeff Thermal Expansion??6.6??
Modulus of
Elasticity Tension??29??
Principal Design Features(主要特點)????300M is a low
alloy, vacuum melted, steel of very high strength. Essentially it is a modified
AISI 4340 steel with silicon, vanadium and slightly greater carbon and
molybdenum content than 4340. 300M has a very good combination of strength (280
to 305 ksi), toughness, fatigue strength and good ductility. It is a through
hardening alloy.??
??
Applications (應用范圍)?? Applications for 300M steel
are those that require strength in the 290 - 300 ksi range, such as aircraft
landing gear, high strength bolts and airframe parts.??
Machinability
(加工性能)?? Machining is best accomplished with the alloy in the normalized or
normalized and tempered condition. Final machining to finish tolerances is done
by grinding with care due the hardness of the heat treated alloy (Rockwell C
55). It is important to do a stress relief anneal at 550 F after finish
grinding.??
??
Forming (成形性能)?? Formability by conventional methods is
good in the annealed condition. The alloy behaves much like AISI 4340
steel.??
Welding (焊接性能)?? 300M can be welded by fusion methods or by
flash resistance welding. Approved procedures must be used for fusion welding,
including pre and post-heating practice, because the alloy will air harden due
to heat input from welding. Following welding it is essential to re-normalize or
re-normalize and temper prior to the final hardening heat
treatment.??
??
Heat Treatment??(熱處理)??300M must be normalized at 1700 F
before hardening. After the normalizing treatment the alloy is hardened by
heating to 1600 F and oil quenching. Tempering is then done
last.??
Forging(鍛造性能)????No data. The alloy is forgeable - contact the
supplier for details.??
??
Hot Working (熱工性能)?? No data. Heat input can
cause this alloy to air harden. Contact the alloy supplier for information as to
the advisability of hot working.??
Cold Working(冷工性能)????In the annealed
or normalized condition the alloy has good ductility and can be readily cold
worked by conventional methods.??
??
Annealing(退火)????Anneal at 1550 F and
slow furnace cool at a rate of less than 50 F per hour down to 600 F. From there
it may be air cooled.??
Aging??(時效)??Not applicable to this
alloy.??
??
Tempering (淬火)??Temper at 600 F to give a nominal 300 ksi
strength.??
??
Hardening????300M hardens from cold working and by heat
treatment. See "Heat Treatment" and "Tempering".??
Other Comments????300M
may be joined by Nicer brazing, copper brazing and silver brazing. ?